woven bag color printing ink is not firmly adhered

Date:2018-09-23 Click:0
cause of issue:
1. The surface of the substrate and the surface of the film or woven bag are too smooth (untreated or poorly handled).
2. Ink complexes (ie, auxiliaries) are improperly used or insufficiently used.
3. The dissolved hydrogen bonding force of the ink body < is too different from the dissolved hydrogen bonding force of the woven bag substrate.
Method of exclusion:
1. The surface of the woven bag substrate reaches about 38 dynes.
2. Add 5% chlorinated paraffin before stretching the woven silk.
3. Ink selection should be very careful (same nature).
4. The use of ink should be appropriate, as long as the viscosity is small and the resin content of the ink system is high.
5. Increase printing pressure.